Forging Defects: Types, Causes, Detection and Prevention

Red hot forging lifted by crane in the forging shop, Sharma Technocast

Short answer: forging defects come from three places, and knowing which one tells you how to prevent them. The starting material brings pipe, segregation, inclusions and hydrogen flakes. The forging operation adds laps, underfill, mismatch, internal bursts and surface cracks. Heat treatment adds quench cracks, soft spots, distortion and grain growth. Surface defects are found by visual inspection, magnetic particle (MPI) or dye penetrant (DPT); internal defects by ultrasonic testing (UT); wrong properties by hardness and mechanical tests. Almost every defect is prevented the same way: the right starting material, enough forging reduction, the correct temperature window, a sensible part design, and an inspection plan agreed before production starts.

This guide is written from the forging floor. It lists each defect, what causes it, how it is found and what stops it happening, then sets out what to put in your enquiry so defects are caught before the part reaches you rather than after.

Where Forging Defects Come From

A forged part passes through four stages, and each one can introduce its own defects: the ingot or billet it starts as, the heating, the forging itself, and the heat treatment afterwards. Machining only reveals defects; it rarely causes them.

Infographic showing the three origins of forging defects: material defects such as pipe, segregation, inclusions and flakes; forging defects such as laps, underfill, mismatch, bursts and surface cracks; and heat treatment defects such as quench cracks, soft spots, distortion and grain growth
The three origins of forging defects. Finding the origin is how you stop the defect repeating.

1. Defects That Come From the Starting Material

These are already in the steel before it is heated. Forging can spread them, close them or expose them, but it cannot remove them.

Pipe and shrinkage cavity

As an ingot solidifies, the last metal to freeze sits at the top and leaves a funnel-shaped cavity called pipe. If too little is cropped from the hot top, that cavity is forged into the part and shows up as an internal void or a crack along the axis. It is the classic reason a large shaft fails ultrasonic testing down the centreline.

Prevention: crop enough from the ingot top and bottom, and work the material hard enough that any remaining centreline porosity is closed by the forging pressure. This is why a minimum forging reduction ratio is worth specifying on critical parts.

Segregation

Carbon, sulphur and phosphorus do not distribute evenly as an ingot freezes. The result is bands of different composition, so hardness and strength vary within one part. On a macro-etched section it appears as a pattern of darker and lighter zones.

Prevention: a cleaner melting route, soaking long enough at temperature, and enough reduction to break up the as-cast structure.

Non-metallic inclusions

Oxides and sulphides from steelmaking are drawn out into long stringers as the metal is worked. They lower ductility and impact strength across the grain flow, and clusters of them show up as ultrasonic indications.

Prevention: specify the steel quality, and where it matters, the melting route and an inclusion rating. On parts tested transversely, inclusion content is often what decides whether the test passes.

Hairline cracks (flakes)

Hydrogen dissolved in the steel collects at internal interfaces as the forging cools and opens tiny internal cracks. They are more common in large alloy-steel forgings, and they are invisible from outside: ultrasonic testing or a fracture face is how they are found.

Prevention: use low-hydrogen (vacuum degassed) steel for heavy sections, and cool slowly after forging, holding the part so hydrogen can diffuse out before it does damage.

The practical point: material defects are bought, not made. They are decided when the steel is ordered, which is why the grade, the specification and any melting or cleanliness requirement belong in the purchase order, not in a conversation after the forging fails.

2. Defects That Come From the Forging Operation

These are the defects a forge controls directly, through temperature, die design, preforming and how the metal is worked.

Laps and folds

Metal folds over on itself and the two surfaces never weld, because an oxide layer sits between them. Caused by too much metal in the preform, sharp corners, or a shape that makes the metal double back. Found visually or by MPI, and usually running along the surface.
Prevention: correct preform, generous radii, die design that lets metal flow one way.

Underfill (unfilled section)

The die cavity does not fill, so a corner or a rib comes out short. Caused by too little starting material, metal that is too cold, too few blows, or a preform that puts the volume in the wrong place.
Prevention: correct billet weight, the right temperature at the moment of forging, and a preform matched to the part.

Die shift and mismatch

The two die halves are not aligned, so one side of the part is offset from the other across the parting line. It is a dimensional defect, found by measuring across the parting line.
Prevention: aligned and guided dies, well-maintained equipment, and a mismatch tolerance agreed in advance. Tolerances for steel die forgings are commonly specified to EN 10243-1.

Internal and centre bursts

The inside of the part tears while the outside looks perfect. Caused by working the metal too cold, reducing too hard in one pass, or dies that grip only the surface so the centre is pulled apart rather than squeezed. Found only by ultrasonic testing or by sectioning.
Prevention: stay inside the temperature window, plan the reduction per pass, and use dies that work the centre of the section, not just its skin.

Surface cracks

Cracks that open on the outside while forging. Caused by working below the safe temperature range for the grade, by too rapid a temperature change, or by hot shortness when the steel is held too hot.
Prevention: control the furnace, reheat between stages rather than forcing a cold part, and keep to the grade’s forging range.

Overheating and burning

Overheating coarsens the grain and lowers toughness; it can usually be corrected by normalising. Burning is worse: the grain boundaries begin to melt and oxidise, and the damage is permanent. A burnt forging is scrap.
Prevention: furnace control and soak times matched to the section, not to the clock.

Scale pits

Oxide scale forms in the furnace and is pressed into the hot surface by the dies, leaving shallow pits once it falls away. They matter when the surface is a finished surface.
Prevention: descale between heats, control the furnace atmosphere, and leave enough machining allowance.

Decarburisation

Carbon burns out of the surface layer during heating, leaving a soft skin that will not harden properly. It is a problem on parts used as forged, or where the hardened surface does the work.
Prevention: limit time at temperature, control the atmosphere, and leave machining stock so the affected layer is cut away.

Grain flow in the wrong direction

This one is not a flaw in the metal but a flaw in the design. Forging lines the grain up with the shape of the part, which is most of the reason forgings outperform parts cut from bar. If the die shape, or later machining, cuts across that flow at a highly stressed point, the part is weaker exactly where it needs strength. It passes every inspection and still fails in service.

Prevention: design the forging so the flow follows the loaded direction, and keep enough stock that machining does not cut through it. A macro-etched section is how grain flow is checked.

3. Defects That Come From Heat Treatment

The forging can be perfect and still be ruined afterwards. Heat treatment is where hardness, strength and toughness are set, and where a good part is most easily lost.

Defect What causes it How to prevent it
Quench cracks Cooling too fast for the grade and section, sharp corners and sudden changes of section, or quenching from too high a temperature Match the quench medium to the steel’s hardenability, radius every corner, temper without delay after quenching
Distortion Uneven cooling, long or thin sections, residual stress from forging Support the part in the furnace and the quench, normalise before hardening, allow straightening and stress relief in the route
Soft spots and low hardness Uneven quenching, a section too heavy for the grade’s hardenability, or a decarburised skin Choose a grade that hardens through the section, agitate the quench, test hardness at the specified position
Coarse grain Austenitising too hot or holding too long Control temperature and soak time; normalise to refine the grain before the final treatment
Temper embrittlement Holding or slow cooling Cr-Mo steels such as 4140 and F22 through roughly 375 to 575 °C Cool quickly through that range after tempering; on critical parts, specify a step-cooling or embrittlement test

How Each Defect Is Found

No single test finds everything. A sound inspection plan combines a surface method, a volumetric method and a properties check. These are the methods used on steel forgings, and what each one is good for.

Chart matching forging defects to the inspection method that finds them: visual and dimensional, magnetic particle, dye penetrant, ultrasonic testing, hardness testing, mechanical testing and macro-etching
Which inspection method finds which defect. Surface, internal and property defects each need a different test.
Method Finds Notes
Visual and dimensional Underfill, mismatch, scale pits, visible laps, distortion The cheapest check and still the one that catches most of what goes wrong
Magnetic particle (MPI) Surface and slightly subsurface cracks and laps For magnetic steels only. Commonly specified to ASTM A275 for forgings
Dye penetrant (DPT) Surface cracks open to the surface Used on stainless and duplex grades, where MPI will not work
Ultrasonic (UT) Pipe, cavities, bursts, flakes, inclusion clusters The only practical way to inspect the inside of a heavy forging. Commonly specified to ASTM A388
Hardness Wrong or uneven heat treatment, soft spots, decarburised skin Specify the test position: surface hardness and mid-radius hardness are not the same number
Tensile and impact Strength, ductility and toughness Taken from test material heat treated with the forging. Specify the orientation, since transverse results are lower
Macro-etch Grain flow, segregation, bursts, the remains of pipe A sectioned and etched sample; commonly specified to ASTM E381
Microscopy Grain size, depth of decarburisation, inclusion rating A polished sample under the microscope

How We Control This at Sharma Technocast

Our forging facility works on 5,000 T and 1,500 T hydraulic presses with manipulators, plus closed die, hammer and roll forging lines and an in-house die shop., plus closed die, hammer and roll forging lines and an in-house die shop. Gas-fired furnaces up to 1,400 °C heat the stock, and heat treatment runs in bogie furnaces with polymer and oil quench tanks. Forgings go up to 30 t: shafts to Ø 2,000 mm and 16 m long, rings and tube sheets to Ø 3,000 mm.

On the inspection side we run four ultrasonic flaw detectors, magnetic particle and dye penetrant equipment, a 200 kN universal testing machine, an impact tester, a Brinell hardness tester, a metallurgical microscope with image analysis and a profile projector. Chemical analysis is carried out by an external testing laboratory. Chemical, mechanical, ultrasonic, MPI and DPT testing are done for every heat or batch as the order requires, and the certificates travel with the parts.

We forge EN8, EN19, EN24, AISI 4130, 4140 and 4340, ASTM A105 and A350 LF2, ASTM A182 F11, F22, F304, F316 and F51, hot die steels and aluminium 6061. Grade by grade, the chemistry and heat treatment are set out in our forging materials guide.

What to Put in Your Enquiry So Defects Are Caught

Most arguments about forging quality are really arguments about something that was never written down. These eight lines prevent nearly all of them.

  1. Grade and specification, including the class or condition, not just the number on the drawing.
  2. Heat treatment condition and the mechanical properties required, with the test position and orientation.
  3. Minimum forging reduction ratio, on heavy or critical parts.
  4. Ultrasonic testing: the standard, the stage at which it is done, and the acceptance level.
  5. Surface inspection: MPI or DPT, and to which acceptance standard.
  6. Hardness: the range and where it is measured.
  7. Delivery condition: as forged, rough machined or finish machined, and the machining allowance.
  8. Documents: the certificate type, and whether a third party has to witness anything.

Agreeing these before production means the forge builds the inspection into the route instead of testing at the end and hoping. For large one-off parts, see open die forging; for repeat parts made in a die, see closed die forging; and for the tolerances to expect, see forging tolerances.

Cast parts fail for different reasons, with different tests and different remedies. For those, see our guide to casting defects: types, causes, remedies and prevention.

Have a forging that keeps failing inspection?
Send us the drawing, the grade and the rejection report. We will tell you which stage the defect comes from and what to change.

Ask our forging team

Frequently Asked Questions

What are the most common forging defects?

Laps and folds, underfill, die shift or mismatch, surface cracks, scale pits and decarburisation are the ones seen most often, because they come from the forging operation itself. Internal bursts, pipe and hydrogen flakes are less common but more serious, because they cannot be seen from outside and are only found by ultrasonic testing.

What causes cracks in forgings?

It depends where the crack is. Surface cracks usually mean the metal was worked outside its safe temperature range, or cooled too suddenly. Internal cracks usually mean either a burst from working the centre too hard or too cold, a hydrogen flake from the steel itself, or a quench crack from heat treatment. Finding where the crack sits, and whether it followed the grain flow, is how the cause is identified.

Can forging defects be repaired?

Some can. Shallow surface defects can be ground out if enough machining allowance remains and the part still meets its drawing. Overheated grain structure can often be corrected by normalising. Weld repair is possible only when the specification allows it and under an approved procedure. Burnt material, through-thickness cracks and flakes cannot be repaired; those parts are scrapped.

What is the difference between a lap and a crack in forging?

A lap is metal folded over itself during forging, with oxide trapped in the fold, so it never bonds. It usually runs along the surface at a shallow angle and follows the direction the metal flowed. A crack is a break in sound metal, usually running into the part rather than along it. Both show up under magnetic particle inspection, but they have different causes: a lap points to the die and preform design, a crack points to temperature or heat treatment.

How are internal defects in forgings detected?

By ultrasonic testing, usually after rough machining and heat treatment so the sound path is clean and the structure is final. The standard most often specified for steel forgings is ASTM A388. Where a part is sectioned for approval, macro-etching shows grain flow, segregation and the remains of pipe directly.

Does forging remove defects in the starting material?

Partly. The pressure of forging closes internal porosity and welds up small cavities, and working the metal breaks up the coarse as-cast structure, which is why a minimum reduction ratio is worth specifying. But forging cannot remove inclusions, segregation or hydrogen. Those are elongated and redistributed, not eliminated, so they have to be controlled when the steel is bought.

What is decarburisation and why does it matter?

It is the loss of carbon from the surface layer while the steel is hot in the furnace. The affected skin has less carbon than the steel underneath, so it will not harden to the same level and is softer than the drawing expects. It matters on parts used as forged and on parts where the surface carries the load, such as gears and shafts. Leaving enough machining allowance removes the affected layer.

How do you prevent forging defects?

Control four things. Buy the right material for the section and the duty. Heat and forge inside the grade’s temperature window, with enough reduction to work the centre and not just the surface. Design the part for forging, with generous radii, a sensible parting line and grain flow that follows the load. Then heat treat and inspect to a plan that was agreed before production, not after the first rejection.

Forging
View Next Page >>